    Some anodizing I did for the faceplate of the new Audio Sensibility speakers!
This is a solid slab of 6061 aluminum. This was polished to a mirror finish then anodized using a special process I have to keep maximum shine in black.
    These guys  also upgraded some speakers that I mentioned in an earlier post.
Sounds amazing!
     Check out their website...well known for the best audio cables:
http://audiosensibility.com

Thursday, May 12, 2016

Precision Billet Brake Levers and Crank Bolts

    Precision Billet brake levers are now complete.
These are logo free and can be purchased at www.torontocycles.com and will be soon updated at www.precisionbillet.com. We will be doing some custom anodizing, splash and streak. Soon we should have custom laser engraving but might be a few months away.
    Titanium crank bolts with press on collars will be done shortly: photo below.


Tuesday, March 22, 2016

Anodizing Mirror Polish

Just some pics of mirror I did on the black part in the center. Reflection is some parts and a bike hanging from the ceiling. The purple on the left is overcast with black (not polished) and looks black at discrete angles. I'll follow up sometime about polishing aluminum. Mirror anodizing is a slightly different technique.

Friday, March 11, 2016

Precision Billet Purple Derailleur Mounted

This is a Purple precision Billet rear derailleur mounted. Pics from a customer "Robert", we did some custom anodizing for him on this.
 
 

Tuesday, March 8, 2016

Anodizing Tips: Silver

    Silver is very easy to anodize since there is no color added. The base finish, like all anodizing will have a large result on the finish. I like polished as much as possible. If you have a mirror finish the anodizing will tend to pull the grains out of the mirror finish but should reflect really well. Blasted or etched will look whiter. The photo isn't that great (hard to take pics of silver) but you can see the reflection of the black pipes in the part.
    A few little tricks: I do short anodizing time, about half needed for dye. To check the surface (Since bleach testing wont work), after sealant, use mother's aluminum polish. if anodized it will not blacken. On sealant I just use boiling water as most sealants have a tinge of green. Totally fresh water too as any residue dye can soak in and cause a cast of color.
    A few drops of blue is a little trick I have found. In person (camera make it look yellowish)  the above part has a blue tinge. The eye sees blue in the spectrum as silver and this helps offset yellow and grey casting in the part.

Friday, February 26, 2016

New Website: Revolver Toys

We have opened a new website for some toys that we will be producing. This is geared at the executive end of the market with high quality cnc desktop toys. The website is in development and will be a very simple site.

Friday, February 5, 2016

Anodizing Tips: Calling in the Store for Advise

      I've been getting too many calls into the store for setup on anodizing. There's a few issues that I almost always encounter. I placed these below and some rules to the process. Anodizing is really complex and too much time can be wasted. I'm very busy and the long phone calls isn't my thing.
1. Almost nobody has read the setup and tips I post on the blog before calling.
2. Almost everyone tells me what they read somewhere else, often times these things make no sense. Many forum people have no experience or will intentionally advise wrongly in order to deter future anodizers. I already know how to anodize so informing me of what you have heard doesn't mean much to me.
3. I will always ask the following so please know this: Volts, Amps, Tank temperature, Acid ratio, Time, Part Size, Type of aluminum (if you know...not all alloy is the same). I will also ask what you have purchased from the www.anodizeworld.com website. I reserve advise for paying customers only. I cannot help if you have no info on your setup...know the above!
4. Please have a pencil and paper so if I advise you on the phone you remember and don't need to keep calling back asking the same questions.
5. If you like to do a way other than I advise then I cannot help. Arguing with me on the phone is not good.
6. I cannot spend an hour micro-detailing the process.
    Rookie Problems:
#1 Not reading what I have posted / Ignoring what you have read.
#2 Acid is way too strong in ratio
#3 Using constant amps
#4 Way over complicating the process / Overthinking
#5 Lack of patience
#6 Arguing with experienced people.

Monday, January 25, 2016

Anodizing Tips: Nitric Acid

   Nitric Acid is used in anodizing to remove heavy metals. Most notably Copper and Zinc but more so copper. Aluminum always has different elements alloyed with it to give strength and in anodizing we do not want these contaminants.
     Anodized metals that are alloyed with copper give a great anodize and also gives a hard glossy shell like appearance if done properly. The problem is too much copper is usually left after phosphoric de-smut. Too much copper left can give black streaks and spots. The parts to the right have copper content (Not the 6061). Note the glossy finish but no blackening on the gold part. The 7075 parts feel slick to the touch. this is assisted by a 10% nitric acid dip for about 5 minutes, followed by a hot water blast and re-dip. The hot water helps wash the surface.
    Nitric Acid is the only acid that will aggressively attack copper and the noble metals. It's not so aggressive on aluminum so can give a shine boost if done properly. It will also aggressively attack eyes, skin and clothes much worse that sulfuric. It also fumes badly if heated and is a requirement in brite dip. The fumes on reaction with copper is strong and produces Nitrogen Dioxide or Mustard Gas...not good. For this reason we only sell reduced to 35% and has to be shipped surface hazard material. At this level it wont fume out and greatly reduces risk.
    

Wednesday, January 13, 2016

Precision Billet Jockey Wheels

Precision Billet jockey wheels new for 2016.
These will fit vintage Proshift / Precision Billet / Paul and most other derailleurs including Shimano. These are all made in Canada and anodized in house. These have a metal shielded ball bearing for easier spinning.
ID is for 5mm bolts.
Total width including caps is 8mm.
Gold side caps only.
8 grams per pulley.
Currently for sale on Toronto Cycles website and will be added to Precision Billet site shortly.

Saturday, January 2, 2016

Anodizing Tips: Setup Parameters

I've been asked many times about the basic parameters for type 2 anodizing. below I will list the voltages, temperatures and basic information that I use for anodizing. This tip page does not include dyes, dyes and de-smut will be a later topic).
   
Green AEN
Term used: Dissolution = When the acid eats back the anodized coating faster than the end current can produce.

Jet Black Anodizing
    Voltage: I run at 14.2 to 14.8 volts. This can vary a bit depending on the acid strength and tank temperature. Warmer tank = lower voltage. If the voltage is too high the parts will start to burn. If the parts burn at 14.0 volts then the acid is too strong. If the acid is too strong than pitting (Severe burning) will occur.
    Amps: Amps will self regulate. Amps must fall during the process. Amps will fall fastest at first then slow down. The final value to dissolution will be about 70 - 75% of the starting amps after 5 minutes). In other words if the starting amps after 5 minutes is 2.0 then will be anodized fully at 1.4 to 1.5 amps.
    Time: I go 1 hour 10 minutes. I go less on silver. Going longer time will hit dissolution. Really it's only necessary to go as much time as needed to take full dye and no burning.
Hot Pink
    Temperature: 70 degrees. Some dye wont take with cooler tanks (Grey BL, Pink, Reds I've had issues with cooler tanks). Warmer tank = lower voltage.
    Agitation: I use a wave maker. I don't like the bubble method but some feel is ok.
    Acid: Sulfuric acid at a 10-15% ratio. There is a 720 rule or formula but I don't use it. Really complicated and how to find the surface area of a bolt? Change the bolt and new formula...hmmm. Most rookies start with way too strong acid bath. I use a hydrometer value of 1.4 baume.
    This step is the hardest to get. My advice is a 10% bath and follow the above values. If it's too weak add a bit of acid. Remember its much easier to add acid then the split the tank to reduce.
     New acid tanks can burn parts easier. Adding some aluminum matures the tank and helps resist burn. I add phosphoric and oxalic acid in very small amounts but isn't needed. This can help burn and black tracks. Clean Tanks are very important...I will follow up on this later.
We have more tips and sell supply on www.anodizeworld.com